[1]曹新民.铸造起重机Z形臂的开裂失效分析[J].特种铸造及有色合金,2020,40(07):746-748.
Cao Xinmin. Failure Analysis of Crane Z-arm Fracture[J]. Special Casting & Nonferrous Alloys, 2020,40(7):746-748.
利用直读光谱仪、拉伸试验机、布氏硬度计和扫描电镜对开裂的Z形臂进行了检测。结果表明
Z形臂的成分、组织、性能均满足技术要求。断口的微观组织由胞状晶和树枝晶、气孔以及等轴形韧窝组成
分析发现
Z形臂在铸造过程中形成的冷隔缺陷
是导致开裂的主要原因。通过采取控制浇注时间和浇注温度以及增加冒口的措施
取得了良好的效果。
The cracked Z-arm was tested by direct reading spectrometer
tensile tester
Brinell hardness tester and scanning electron microscope.The results show that the composition
structure and performance of Z-arm meet the technical requirements.The micro-morphology of the fracture presents cellular crystal
dendrite
pore and equiaxed dimple.The Z-arm is not fully fused in the casting process
resulting in the formation of cold shut
which is also the main reason of the cracking.Through the control measures of limiting pouring time
measuring pouring temperature and adding riser
effective improvement could be achieved.