The cleaning strainer base of 280 diesel engine in low pressure casting was discussed.The processing and mould design and trial production were expounded systematically.Some key parameters were set including the pouring temperature of 720~760 ℃
lift time of 5~10 s
filling velocity of 1.2~1.5 m/s
filling pressure of 0.05~0.08 MPa
holding pressure of 0.15~0.25 MPa
holding pressure time of 6~10 min and die temperature.
关键词
ZL101低压铸造柴油机滤清器
Keywords
ZL101Low Pressure CastingCleaning Strainer for Diesel Engine